IRHD Hardness: Test Results
Below you can find the description of the test results produced by Hardness Check software



 

IRHD: IRHD Hardness 
The calculation returns the IRHD Hardness in conformity with ISO 48-2 standard. The Hardness is obtained by measuring the indentation of the indentor after the application of the minor force for 5 seconds and the application of the main force for 30 seconds.

REFERENCE STANDARD: ISO 48-2 / ASTM D 1414

UNIT: IRHD points
RESOLUTION: 0.01 IRHD

CALCULATION PARAMETERS:
Test Time: t (the software permits to set even non standard test times)


Angle Coefficient of Hardness Regression line  
The calculation returns the angle of the Regression Line of the Hardness-Vs-Time Curve plot in Logarithmic axes.
The angle coefficient provides usefull information about the visco-elastic behavior of the sample during the test. Measures performed on the same product can be used to compare the curing level of different samples or technical parts.
The result is obtained automatically during the standard execution of the hardness test.

UNIT: IRHD/sec
RESOLUTION: 0.01 IRHD/sec




Hyst: Hysteresis 
The measure of the Hysteresis is performed by removing the main force at the end of the test time and measuring the sample recovery after the set test time.
If the sample has a completely elastic behaviour, the recovery will be complete and the hardness reading will be 100 IRHD. The actual reading at the end of the test provides an evaluation of the visco-elastic properties of the sample
The measure can be useful to compare the behaviour of different products.
The measurement time after the removal of the sample can be set in the test procedure.
The Hysteresis test is performed completely automatically by the instrument even with instruments performing multiple tests.

UNIT: IRHD
RESOLUTION: 0.01 IRHD


Is: Hysteresis - Energy Loss 
This calculation returns the Hysteresis Energy (ie the energy lost during the execution of the load and unload of the sample during the execution of the irhd hardness test).

The energy loss can be expressed as Energy (N*mm) or as % of the energy applied in the loading cycle.



Gibitre Instruments
Via dell'industria, 18
Bergamo (Italy)
te. +39 035 461146
www.gibitre.it
info@gibitre.it

Copyright Gibitre Instruments
Below you can find the description of the test results produced by Hardness Check software
Campi di applicazione  >  Prove su pneumatici  >  Rheocheck MD - Drive
IRHD
Hardness:
Test Results
hardness irhd formulas: IRHD硬度計:ソフトウェア計算:IRHD硬度。

Below you can find the description of the test results produced by Hardness Check software

Applications

IRHD: IRHD Hardness 

The calculation returns the IRHD Hardness in conformity with ISO 48-2 standard. The Hardness is obtained by measuring the indentation of the indentor after the application of the minor force for 5 seconds and the application of the main force for 30 seconds.

REFERENCE STANDARD: ISO 48-2 / ASTM D 1414

UNIT: IRHD points
RESOLUTION: 0.01 IRHD

CALCULATION PARAMETERS:
Test Time: t (the software permits to set even non standard test times)

hardness irhd formulas: Gibitre-Hardnessソフトウェア。ソフトウェアによる計算。ISO 48-2に従って計算されたIRHD硬度。
Gibitre-Hardnessソフトウェア。ソフトウェアによる計算。ISO 48-2に従って計算されたIRHD硬度。

Angle Coefficient of Hardness Regression line  

The calculation returns the angle of the Regression Line of the Hardness-Vs-Time Curve plot in Logarithmic axes.
The angle coefficient provides usefull information about the visco-elastic behavior of the sample during the test. Measures performed on the same product can be used to compare the curing level of different samples or technical parts.
The result is obtained automatically during the standard execution of the hardness test.

UNIT: IRHD/sec
RESOLUTION: 0.01 IRHD/sec

hardness irhd formulas: Gibitre Hardnessソフトウェア。硬さ対時間の回帰直線の傾きの計算(対数軸)
Gibitre Hardnessソフトウェア。硬さ対時間の回帰直線の傾きの計算(対数軸)

Hyst: Hysteresis 

The measure of the Hysteresis is performed by removing the main force at the end of the test time and measuring the sample recovery after the set test time.
If the sample has a completely elastic behaviour, the recovery will be complete and the hardness reading will be 100 IRHD. The actual reading at the end of the test provides an evaluation of the visco-elastic properties of the sample
The measure can be useful to compare the behaviour of different products.
The measurement time after the removal of the sample can be set in the test procedure.
The Hysteresis test is performed completely automatically by the instrument even with instruments performing multiple tests.

UNIT: IRHD
RESOLUTION: 0.01 IRHD

hardness irhd formulas: 硬度チェックソフトウェア。圧子から力を抜いた後のヒステリシス計算。
硬度チェックソフトウェア。圧子から力を抜いた後のヒステリシス計算。
 

Is: Hysteresis - Energy Loss 

This calculation returns the Hysteresis Energy (ie the energy lost during the execution of the load and unload of the sample during the execution of the irhd hardness test).

The energy loss can be expressed as Energy (N*mm) or as % of the energy applied in the loading cycle.

hardness irhd formulas: Gibitreソフトウェア。結果の計算式。Tensor-Checkソフトウェア。Is_n(n番目のセットサイクルにおけるヒステリシスエネルギー)の計算をグラフィカルに説明。
Gibitreソフトウェア。結果の計算式。Tensor-Checkソフトウェア。Is_n(n番目のセットサイクルにおけるヒステリシスエネルギー)の計算をグラフィカルに説明。
Download
General catalogue mail request

Shore Hardness: Test Results
Vedi anche: 硬度チェックソフト:設定時間におけるショア硬度
See Also   >
News
Call to action
Mail
info@gibitre.it
The good old e-mail
ready for every season
Phone
+39 035 460146
We welcome your calls Monday through Friday from 8:30 a.m. to 5:30 p.m. in your local time zone.
Newsletter
Subscribe
Stay updated
with the last news
of your sector
Local agent
from: -
See the whole list

In your country
in your language
at your service
Gibitre Instruments S.r.l., Via dell'industria 73, 24126 Bergamo Italia, pec@gibitre-instruments.it P. IVA: IT02827900164 CCIAA REA Bergamo: 326486 | ©2018 - 2026 Gibitre Instruments
Optimist.it
Welcome to the Gibitre Instruments web site
Please chose the preferred Cookie Management.
Benvenuti nel sito Gibitre Instruments
Per continuare scegliete la Gestione dei Cookie che preferite.
Cookies policy
For detailed informations about the use of cookies, please read our
Cookies Management Practice.

Gestione dei Cookies
Per maggiori informazioni sui cookie utilizzati consultate la nostra
Procedura sull'Uso dei Cookies.